By CHX Metal Engineering Team · Published 2026-11-23
Passivation is an acid bath, not a coating: nitric at 20-50% or citric at 4-10% strips free iron from the stainless surface and adds nothing. We passivate 303/304/316L parts to ASTM A967, verify by water-immersion or high-humidity test, and ship a per-lot record, from MOQ 1.
The bath does the work, and the bath is where it fails
On a finishing quote, passivation looks like the simplest line item - wash, acid bath, rinse, dry - and it is usually the cheapest. It is also the step we get the most late-stage phone calls about, almost always the same call: the parts arrived certified stainless, sat in a warehouse for a few weeks, and now there are rust freckles on the surface. The trouble nearly never starts on the certificate. It starts in the tank, or more precisely, before the parts reach it.
A passivation bath does one job: it dissolves the free iron sitting on the surface and leaves the chromium-rich oxide film alone. Nitric acid does this at roughly 20–50% concentration; citric acid does it at 4–10% with less aggressive waste chemistry. Nothing is deposited, no layer grows, no hardness is added. That subtraction-only nature is both the appeal and the trap - it means dimensions barely move, and it also means the bath cannot protect the part from whatever iron it picks up afterward.
Free iron is the enemy, not the alloy
Every cutting operation smears a thin layer of iron-rich material across the surface it just machined. On a lathe running 303 bar, the chips are bright, the surface looks clean, but under that shine sits the smeared layer - and free iron rusts in humid air while the base alloy does not. Passivation removes that layer. It does not change what the alloy is, and it cannot fix a drawing that was never achievable.
For a buyer, the practical consequences are two. First, tolerances: the material removed is far below a micrometre, so critical features held at ±0.005 mm come out of the bath unchanged - we have CMM-checked parts before and after on customer request and the shift is inside the measurement noise. Second, drawings: a note that says only “passivate” leaves the whole chain open - which spec, which practice, what cleanliness before the bath, and what proof afterward. The note that works names them: passivate per ASTM A967, citric practice, verify by water immersion.
Why 303 rusts anyway
303 cuts beautifully because it carries sulphur, and the sulphur forms inclusions in the metal. Those inclusions are not free iron and a bath will not remove them - at high humidity they can produce the same freckling buyers mistake for failure. This is alloy behavior, not process failure, and it is the honest first answer to “why is there rust on my passivated 303 parts?”. If the application cannot tolerate any spotting, the fix is a grade change to 304 or 316L at quotation stage, not a harder acid.
The second mechanism is recontamination, and this one is the shop’s fault. Grinding dust from a wheel that also ran carbon steel, deburring brushes used across alloys, a stainless batch slid along a carbon-steel rack - each one lays fresh free iron onto a clean part, and the bath that ran before the contamination is irrelevant. We keep stainless handling separated from carbon-steel tooling and racks, and we re-run batches when the test catches a slip. That has happened here: a lot of 316L fittings went through after a fixture change and the water-immersion check flagged it, so the lot was re-passivated and delivered two days late. Two days was cheaper than a returned container.
Nitric or citric, and what to write in the RFQ
ASTM A967 (with AMS 2700 as the aerospace-side equivalent) lists both nitric and citric practices, and for 300-series machined parts either is sound. Citric is the direction most shops have moved: no nitrogen-oxide fumes, milder waste treatment, shorter bath life but simpler chemistry. Nitric has the longer industrial record and handles heavier heat-tint oxides better, which matters on welded assemblies more than on turned parts. We do not get religious about it; we match the practice to the alloy and the customer’s spec system, and we name it on the lot record either way.
In the RFQ, one line does the work: passivate per ASTM A967, citric practice, verify by water immersion - or whichever practice and test your program requires. If tolerances matter, leave critical features at ±0.005 mm and let unmarked dimensions ride ISO 2768-m; the bath will not touch either. Ask at quotation, and the practice becomes part of the price rather than a surprise line added after the parts are cut.
What we verify, and what ships with the parts
A967 gives three common acceptance tests: water immersion, high-humidity exposure, and salt spray, in rising order of harshness. For most machined components the water-immersion test is proportionate; salt spray belongs where the customer’s environment demands it, not as decoration on a report. Each lot leaves with a record naming the alloy, the practice, and the test result, and the certificate set can travel together with the material certificates so the heat number and the bath record share one trail.
Our plant in Shajing, Bao’an District has machined since 2013 - 220 machines: 100 machining centres with 30 of them 3+2, 50 CNC lathes, and 70 Tsugami Swiss-type units - with 100+ staff and monthly capacity of 5 million pieces. We hold ISO 9001:2015 and ISO 14001:2015, work in 303/304/316L stainless, 6061/7075 aluminium, TC4 titanium, H59 brass and Kovar, take orders from MOQ 1, and deliver prototypes in 3–7 days and production in 7–15. For aluminium parts the corrosion story runs through anodizing instead - our anodizing guide and the surface finishing hub cover that route. Shipping is EXW Shenzhen only - we are happy to recommend reliable freight forwarders.
| Field | CHX Metal |
|---|---|
| Location | Shajing, Bao'an, Shenzhen, China - 5,000 m² plant, 100+ staff, machining since 2013 |
| Equipment | 220 machines: 100 machining centres (30 of them 3+2), 50 CNC lathes, 70 Tsugami Swiss-type lathes |
| Tolerances | ±0.005 mm on critical features; unmarked dimensions to ISO 2768-m; CMM and optical measurement |
| MOQ | 1 piece |
| Lead times | Prototypes 3–7 days; production 7–15 days; capacity to 5 million pieces per month |
| Materials | 303/304/316L stainless, 6061/7075 aluminium, TC4 titanium, H59 brass, Kovar, engineering plastics |
| Quality | ISO 9001:2015 and ISO 14001:2015; passivation to ASTM A967 with per-lot practice and test records; EN 10204 3.1 certificates |
| Shipping | EXW Shenzhen only - we are happy to recommend reliable freight forwarders. |
Machining capacity behind this article
- Equipment: 220 machines — 100 machining centres (30 of them 3+2), 50 CNC lathes, 70 Tsugami Swiss-type lathes.
- Tolerance: ±0.005 mm on critical features; anything unmarked defaults to ISO 2768-m.
- Volume: up to 5 million pieces a month; prototyping 3–7 days, production 7–15 days.
- Materials: 6061/7075 aluminium, 303/304/316 stainless, H59 brass, copper, TC4 titanium, carbon steel.
- Footprint: 5,000 m² in Shajing, Bao'an, Shenzhen; 100+ staff; founded 2013.
- Terms: EXW Shenzhen only — we are happy to recommend reliable freight forwarders.
Address: Building B, 3rd Floor, Haosan Maozhoushan Industrial Zone, Buyong Community, Shajing Street, Bao'an District, Shenzhen | Tel: +86-755-27427365 | Email: mc@chxmetal.com
Frequently asked questions
Does passivation change the dimensions of a machined part?
Not measurably. Passivation dissolves the free-iron smear left by cutting, which is far below a micrometre of material, so features held at ±0.005 mm come out of the bath unchanged. We have CMM-checked customer parts before and after on request and the difference sat inside measurement noise.
Why did our passivated 303 parts show rust spots after storage?
Two candidates. Sulphur inclusions - the same feature that makes 303 cut freely - can freckle in humid air, and that is alloy behavior a bath cannot remove. The other is free iron picked up after the bath, from carbon-steel racks or shared deburring tools. Ask whether the lot passed a water-immersion test and how stainless is handled on the line.
Should I specify nitric or citric passivation?
Both are sound practices under ASTM A967 for 300-series parts. Citric has milder waste chemistry and no nitrogen-oxide fumes; nitric has the longer record and handles heavier heat-tint oxide, mostly a welding issue. What matters more is naming the practice and the acceptance test in the drawing or RFQ instead of writing just 'passivate'.
What documentation comes with passivated parts?
Each lot carries a record naming the alloy, the ASTM A967 practice used, and the acceptance test with its result - typically water immersion for machined components, salt spray where the environment requires it. There is no order-size gate behind it, since our MOQ is 1 piece, and the records can travel with EN 10204 3.1 material certificates so heat number and bath record share one trail.
Do you also passivate aluminium parts?
No - aluminium takes a different route. Passivation chemistry targets stainless steel; for aluminium we use anodizing, which builds a controlled oxide layer rather than stripping contamination. The choice depends on corrosion exposure, wear and dye requirements, and our anodizing guide walks through Type II, hard anodizing and how film growth moves hole dimensions.
Send your drawings for a DFM review and a quotation
STEP, IGES, DXF, DWG or PDF — note the material, quantity and finish. Quotes usually go back within one working day. Email mc@chxmetal.com or use the quote form.