Electropolishing CNC Stainless Parts: What Comes Off First

By CHX Metal Engineering Team · Published 2026-11-25

Electropolishing is anodic dissolution in a phosphoric-sulphuric bath: it removes 5-25 µm of stainless surface, roughly halves Ra and rounds burrs no brush reaches. We turn and mill at ±0.005 mm, polish through a qualified partner, and verify size and Ra with a CMM on every lot, from MOQ 1.

A thread ring gauge should stop after two or three turns. On a lot of 316L spool bodies that came back from the polisher it walked on by hand - the thread was 9 µm under the low limit on the major diameter. Nothing had been machined wrong. The polishing house ran the batch four minutes longer than the previous one, and on a 6g thread those four minutes show up on a gauge.

Hold on to that: electropolishing is a cutting operation wearing a finishing label. Metal leaves the part, and it does not leave evenly.

What the tank actually does

The part hangs as the anode in a phosphoric-sulphuric electrolyte. Current is applied and the surface gives up metal ion by ion; oxygen forms at the work, hydrogen at the cathodes, so nothing is driven into the part as it is in plating - one reason the process suits thin sections and spring temper. No layer is added.

Removal is not blind, which is the useful part. Current density runs highest at geometric high points, so peaks dissolve faster than valleys. A turned face at 0.8 µm Ra commonly comes out near 0.3, and a burr at a cross-hole edge rounds over instead of being cut off. Targets are quoted between 5 and 25 µm - brightening at the low end, cleanability specs for gas-line or surgical parts at the high end. Ask for microns; “electropolish” alone is not a specification.

The microns come off the edges first

A sharp corner can lose two to three times the nominal removal while a flat face loses one, because the corner carries more current. The casualties are predictable: thread crests, chamfer tips, the first thread of a fine pitch, the knife edge of a seal land, the outside of a wall already springing away from the tool.

So stock first. If a 6g thread must stay 6g, the pre-polish diameter is turned high enough to spend the difference, or the thread is masked - we do the former by default. Bores are the second problem: throwing power falls off with depth, so a Ø3 mm hole 30 mm deep polishes at the mouth and barely at the bottom.

The failure we see too often: “electropolish, Ra 0.4 max” on a feature with a 4 µm tolerance band. The first article comes back oversize and the finish certificate is correct. Both documents are true and the part is scrap.

Ra, burrs, and where 303 fights back

Two selling points are honest. Levelling gives a real Ra drop, typically by half. And the bath reaches edges no brush touches - the intersection of a cross-hole, the inside of a small port, the root of a groove. On anything cleaned between uses, that matters more than the number on the print.

What gets oversold is the idea that polishing hides material problems. On 303 the sulphur that makes the alloy cut freely sits in manganese sulphide stringers, and the bath attacks those inclusions faster than the matrix. The surface comes back looking worse: scattered pits and dark streaks along the bar. A drawing asking for 303 and a mirror finish has the grade wrong, not the tank.

Who owns the tank

Most supplier pages go quiet here. Our electropolish is not in our building. Turning and milling are ours - 220 machines in Shajing, 100 machining centres with 30 of them 3+2, 50 CNC lathes, 70 Tsugami Swiss-type units - and the tank belongs to a qualified partner. A buyer auditing a process needs to know where the part travels.

We control both sides of it: pre-polish Ra and stock off our own lathes, masking of threads and fits, a coupon from each lot, and the dimensional check after. When a lot lands out of band we recut rather than ship with a deviation note - twice this year, most recently a batch of 316L spool bodies 6 µm under on a seal bore.

What to put on the drawing

Three elements carry it. Name the standard - ASTM B912 is the one most drawings reach for - then removal in microns, then the surfaces that must not move: electropolish per ASTM B912, 10-15 µm removal, mask M12x1 thread and Ø8 H7 bore, Ra 0.4 max on sealing faces, verify dimensions after polishing.

Then two questions that expose a weak quote: is the polishing under your roof, and what pre-polish Ra will you start from? The first tells you who to audit; the second whether the shop plans to spend metal or just dip the parts. A quote promising Ra 0.2 from an as-turned 1.6 surface, with no stock mentioned, is quoting a wish.

Where the goal is corrosion resistance rather than brightness, passivation is cheaper and removes no metal at all - our passivation guide covers that call. Electropolishing earns its price where a burr-free, cleanable, low-Ra surface is functional: gas-line and vacuum fittings, surgical components, semiconductor wetted parts, any bore a customer will swab. The VCR fitting article shows it on a 316L part; the surface finishing hub lists the routes side by side.

From our side: prototyping 3–7 days, production 7–15, MOQ 1, ±0.005 mm on the features we hold, up to 5 million pieces a month from a 5,000 m² plant with 100+ staff, machining since 2013, ISO 9001:2015 and ISO 14001:2015. Shipping is EXW Shenzhen only - we are happy to recommend reliable freight forwarders.

FieldCHX Metal
LocationShajing, Bao'an, Shenzhen, China - 5,000 m² plant, 100+ staff, machining since 2013
Equipment220 machines: 100 machining centres (30 of them 3+2), 50 CNC lathes, 70 Tsugami Swiss-type lathes
Tolerances±0.005 mm on critical features; unmarked dimensions to ISO 2768-m; CMM check before and after polishing
MOQ1 piece
Lead timesPrototypes 3–7 days; production 7–15 days; electropolishing adds 3–7 days; capacity to 5 million pieces per month
Materials303/304/316L stainless, 17-4PH, 6061/7075 aluminium, TC4 titanium, H59 brass, Kovar
QualityISO 9001:2015 and ISO 14001:2015; electropolishing to ASTM B912 at a qualified partner, with removal target and post-polish dimensional check
ShippingEXW Shenzhen only - we are happy to recommend reliable freight forwarders.

Machining capacity behind this article

Address: Building B, 3rd Floor, Haosan Maozhoushan Industrial Zone, Buyong Community, Shajing Street, Bao'an District, Shenzhen  |  Tel: +86-755-27427365  |  Email: mc@chxmetal.com

Frequently asked questions

How much material does electropolishing remove?

Typically 5-25 microns, depending on bath time and current. A brightening pass sits near the low end; a cleanability specification for a gas-line or surgical part runs around 10-15 microns. Ask for the target in microns and treat it as a machining allowance, because sharp edges and thread crests can lose two to three times the nominal figure.

Can electropolishing be used to bring a part into tolerance?

Not reliably, and a drawing should never depend on it. Polishing removes metal and removes more from high points, so it drifts away from a tight band rather than settling into one. The workable route is to turn the features with allowance - we hold ±0.005 mm on critical features - and verify dimensions after the bath, masking any thread or fit that cannot move.

Is electropolishing better than passivation?

They solve different problems. Passivation strips free iron from the surface and removes no metal, so dimensions and thread classes are untouched. Electropolishing removes metal, halves Ra and rounds burrs no brush can reach. Where cleanliness or a burr-free edge is functional, polishing earns its cost; where the goal is only corrosion resistance, passivation is cheaper.

Why did our 303 parts come back with pits after polishing?

Because 303 carries sulphur in manganese sulphide stringers, and the bath attacks those inclusions faster than the surrounding matrix. The result is a pitted, streaked surface that looks worse than before polishing. That is a grade problem, not a bath problem - 316L or 304 will polish clean if the application allows the change.

Do you do electropolishing in-house?

No. Turning and milling are ours; the tank belongs to a qualified partner we have used for years, and the turnaround is 3-7 days on top of machining. We control both ends of it - pre-polish Ra and stock from our own lathes, masking, a lot coupon, and the post-polish dimensional check - and we would rather say that than imply a line we do not have.

Send your drawings for a DFM review and a quotation

STEP, IGES, DXF, DWG or PDF — note the material, quantity and finish. Quotes usually go back within one working day. Email mc@chxmetal.com or use the quote form.